3Cr3Mo3VNb(HM3)钢合金元素的构成特点
2.1 3Cr3Mo3VNb钢的化学成份见 (表1) %
C | Cr | Mo | V | Nb | Si ≤ | Mn ≤ | P ≤ | S ≤ |
0.24-0.33 | 2.60-3.20 | 2.70-3.20 | 0.60-0.80 | 0.08-0.15 | 0.60 | 0.35 | 0.030 | 0.030 |
3.1. 线膨胀系数的对比见
几种典型模具钢的线膨胀系数α (×10-6℃-1)与温度的关系 (表2)
温度/℃ | 20-100 | 20-200 | 20-300 | 20-400 | 20-500 | 20-600 | 20-700 |
3Cr2W8V | 14.3 | 14.7 | 15.6 | 16.3 | 16.1 | 15.2 | 15.0 |
4Cr5MoSiV | 10.0 | 10.9 | 11.4 | 12.2 | 12.8 | 13.3 | 13.6 |
3Cr3Mo3VNb | 10.1 | 10.8 | 11.6 | 11.9 | 12.3 | 12.6 | 13.0 |
3.2. 热导率的对比见 表三
几种典型模具钢的热导率λ(W/(m·K ))与温度的关 (表3)
温度/℃ | 20 | 100 | 200 | 300 | 400 | 500 | 600 | 650 | 700 | 850 | 900 |
3Cr2W8V | - | 20.10 | 22.20 | - | - | - | - | - | 24.28 | - | 23.03 |
4Cr5MoSiV | - | 25.96 | 27.61 | 28.47 | 28.05 | 27.63 | 26.77 | - | 25.99 | - | - |
3Cr3Mo3VNb | - | 30.14 | 30.38 | 31.82 | 32.24 | 32.66 | 32.66 | - | 32.66 | 32.66 | - |
H13 | 32.33 | - | - | - | - | - | - | 28.89 | - | - | - |
3.3. 临界点的对比见 表四
几种热模锻典型模具钢的临界温度(Ac1、Ac3、Ar1、Ar3和Ms) (表4)
临界温度/℃ | Ac1 | Ac3 | Ar3 | Ar1 | Ms |
5CrNiMo | 720 | 820 | - | 690 | 210 |
3Cr2W8V | 800~850 | 850 | - | 690~750 | 380 |
4Cr5W2SiV | 800 | 875 | 840 | 730 | 275 |
3Cr3Mo3VNb | 836~948 | - | - | 771~923 | 390 |
4Cr5MoSiV1(H13) | 850 | 915 | 815 | 775 | 340 |